Materials · alloy steels
4140 vs 4340 steel: differences, conditions (annealed, prehardened) and machining
4140 (chromium-molybdenum) and 4340 (with nickel): hardenability, toughness, section sizes, delivery conditions (annealed, prehardened 28–32 HRC), machining, welding with preheat, and how to choose.
4140 and 4340 are the two most common alloy steels in machine shops for shafts, pins, tooling and stressed parts. Both contain chromium and molybdenum; 4340 adds nickel (about 1.65 to 2.0% per the AISI/SAE composition), which raises hardenability (through-hardness in heavy sections) and toughness.
Comparison
| Criterion | 4140 | 4340 |
|---|---|---|
| Alloying elements | Cr, Mo | Ni, Cr, Mo |
| Hardenability | Good | Higher: better through-hardness in large sections |
| Toughness / fatigue | Good | Higher at equal strength |
| Cost | Lower | Higher |
| Machinability | Good when annealed | A bit harder, more tool wear |
| Typical uses | Shafts, pins, tool holders, fixtures, medium parts | Fatigue/impact-critical parts, heavy sections, aerospace, heavy tooling |
Delivery conditions
| Condition | Description | For whom |
|---|---|---|
| Annealed | Softest, best machining | Parts to be quenched and tempered after machining |
| Pre-hardened (“4140 HT”) | Quenched and tempered at the mill, often around 28–32 HRC | Finished parts with no later heat treatment |
| Normalized | Uniform structure | Per specification |
Machining approach
- Pre-hardened: machine straight to size; carbide tools, more conservative conditions than annealed (see Feeds and speeds).
- Annealed + heat treat after: rough, leave stock, quench and temper, then grind or finish tight dimensions (possible distortion in hardening).
- Stress relieve between roughing and finishing if the part is long or asymmetric.
Welding
Both steels are hardenable: without precautions the heat-affected zone can harden and crack. Procedures usually call for preheat, interpass temperature control, matching filler metal and sometimes post-weld heat treatment. Follow a qualified procedure; see Weld preparation.
Choosing
- Medium part, normal loading, tight budget → 4140 (often pre-hardened).
- Large section that must through-harden, critical impact or fatigue → 4340.
- When in doubt: the designer’s specification (and the cited standard) wins.
Common mistakes
| Mistake | Consequence |
|---|---|
| Welding 4140 without preheat | Cold cracking |
| Finishing to size before hardening | Distortion out of tolerance |
| Ordering “4140” without a condition | Annealed stock delivered for a part that needed to be hard |
| Using 1018 speeds | Rapid tool wear |
Ordering checklist
- Grade and condition (4140 annealed, 4140 HT, 4340 annealed…)
- Required hardness and how it’s verified
- Mill certificate
- Allowance if heat treatment follows
- Compare published prices in the price comparison tool
FAQ
Can pre-hardened 4140 be hardened further?
Yes with a new full heat treatment, but you buy pre-hardened precisely to avoid heat treating after machining.
4140 or 4130?
4130 has less carbon: better weldability (chassis tubing), lower achievable hardness.
Sources
- Noramark — 4140 vs 4340 steel, consulted November 26, 2026.
- B&R Production — 4140 and 4340 steel machining guide, consulted November 26, 2026.
- Springer — Heat treatment effects in AISI 1040, 4140 and 4340 steels (review), consulted November 26, 2026.
One guide a week, French-first