Materials · PH stainless
17-4PH stainless: conditions A, H900, H1025 and H1150, machining and aging
What 17-4PH (UNS S17400) conditions mean, when to machine (in condition A, before aging), dimensional contraction on aging, and which condition to choose between hardness and toughness.
17-4PH (UNS S17400, “type 630”) is a precipitation-hardening martensitic stainless: it ships solution-treated (condition A), is machined in that state, then aged at low temperature to reach the required hardness. The condition name gives the aging temperature in °F.
The conditions
| Condition | Aging (per producer data sheets) | Character |
|---|---|---|
| A | Solution-treated, not aged | As-delivered; machines like a 302/304 austenitic stainless per AK Steel |
| H900 | 900 °F (482 °C), 1 h, air cool | Maximum hardness and strength, lowest toughness, hardest to machine |
| H1025 | 1025 °F (552 °C), 4 h | Compromise |
| H1075 | 1075 °F (580 °C), 4 h | Tougher |
| H1150 | 1150 °F (621 °C), 4 h | Toughest and easiest to machine of the aged conditions |
| H1150M, H1150D | Double treatments | Maximum toughness, special uses |
Exact properties per condition (yield, hardness, impact) are in Cleveland-Cliffs (formerly AK Steel) and Carpenter (Custom 630) data sheets.
When to machine
- Rough and finish in condition A if the tolerance allows for contraction.
- Age to the required condition.
- Grind or lightly finish tight dimensions after aging.
Producers state a contraction on aging from condition A: about 0.00045 mm/mm for H900, 0.00053 mm/mm for H1025 and 0.0022 mm/mm for H1150 (Armco 17-4 PH data sheet). On a 100 mm part, that’s roughly 0.05 mm to 0.22 mm depending on condition — plan for it in stock allowances.
Machining in practice
- Condition A: tools and conditions of a 304 stainless (see Stainless: 303, 304, 316) — firm feed, no rubbing.
- H900: high hardness, fast tool wear; carbide, reduced speeds, rigid setup.
- H1150: easier than H900; a common reason to choose H1150 when strength is sufficient.
Choosing the condition
| Need | Condition often chosen |
|---|---|
| Maximum hardness and strength, little impact | H900 |
| Strength / toughness compromise | H1025 |
| Toughness, stress-corrosion cracking resistance, easier machining | H1150 |
The designer owns the choice: the condition must be on the drawing (e.g. “17-4PH, AMS 5643, H1025”).
Common mistakes
| Mistake | Consequence |
|---|---|
| Finishing to size in condition A without allowing for contraction | Tight dimensions out of tolerance after aging |
| Machining in H900 “because it’s simpler” | Tools consumed, long cycle times |
| Mixing up 17-4PH and 304 in stock | Part can’t harden or wrong corrosion behaviour |
| Not stating the condition on the PO | Material arrives in an unexpected state |
Checklist
- Delivery condition (A) confirmed by the certificate
- Final condition on the drawing
- Allowance for contraction and finishing
- Heat treatment by a qualified subcontractor, with report
- Hardness checked after aging if required
FAQ
Is 17-4PH magnetic?
Yes: it is a martensitic stainless, unlike annealed 304/316.
Can it be welded?
Yes with a suitable procedure, often followed by heat treatment; see the producer’s data sheet.
Sources
- Cleveland-Cliffs — 17-4 PH stainless steel product data (PDF), consulted November 26, 2026.
- Armco / AK Steel — 17-4 PH data sheet (PDF), consulted November 26, 2026.
- Noramark — How is 17-4 PH stainless heat treated?, consulted November 26, 2026.
- Production Machining — Dimensional contraction of 17-4 PH stainless steel, consulted November 26, 2026.
One guide a week, French-first
New guides, used equipment in Quebec and price moves. No third-party ads.