Shop · tooling
Cutting tool life: reading wear, extending it and managing it
Flank wear, crater, built-up edge, chipping, notch, plastic deformation: how to recognize each mode, its cause and fix, the dominant role of cutting speed, and a simple shop tracking system.
A tool always wears; the question is how and how fast. Per Sandvik Coromant, flank wear, steady and predictable, is the desirable mode and often serves as the end-of-life criterion. Every other mode signals a problem to fix.
Reading wear
| Mode | What it looks like | Typical causes | Fix |
|---|---|---|---|
| Flank wear | Even wear band below the edge | Normal wear; too fast if speed is too high | Reduce speed, more wear-resistant grade |
| Crater | Hollow on the rake face | Diffusion/chemistry at high temperature (high speed) | Reduce speed, suitable coated grade |
| Built-up edge (BUE) | Material welded on the edge | Sticky materials (aluminum, stainless, copper), speed/temperature too low | Raise speed, sharper edge, lubrication |
| Chipping | Small chips off the edge | Interrupted cuts, vibration, edge too fragile | Tougher grade, stronger edge prep, rigidity |
| Notch wear | Notch at depth-of-cut line | Work hardening (stainless, superalloys), scale | Vary depth of cut, smaller lead angle |
| Plastic deformation | Sagging edge | Excessive temperature and force | Reduce speed/feed, harder grade |
| Thermal cracks | Cracks perpendicular to the edge | Thermal shock (intermittent coolant) | Continuous coolant or dry per recommendation |
What wears most: speed
Sandvik Coromant states tool life depends mostly on cutting speed, then feed, and little on depth of cut. Taylor’s equation (V × Tⁿ = C) formalizes the link; useful for reasoning, but limited: newer models add feed and chip thickness.
In practice: to gain tool life without losing productivity, lower speed a little and raise feed (within tool and finish limits).
Improvement approach
- Look at the worn edge with a loupe (×10) and identify the mode.
- Fix the cause (table above), one parameter at a time.
- Measure tool life (parts, minutes in cut or length machined).
- Standardize: the chosen value goes into the CAM tool library and the setup sheet.
Simple tracking system
| Data | Why |
|---|---|
| Tool reference + grade | Compare suppliers |
| Material machined | Tool life only means something per material |
| Speed, feed, depth | Reproduce conditions |
| Parts or minutes per edge | Main indicator |
| End-of-life mode | Spot problems (chipping ≠ normal wear) |
Common mistakes
| Mistake | Consequence |
|---|---|
| Waiting for breakage to change the tool | Scrapped part, damaged holder |
| Reducing feed to “spare” the tool | Rubbing, work hardening, faster wear |
| Ignoring runout | One flute does all the work |
| Changing grade without recording conditions | No valid comparison |
Checklist
- Rigid setup, minimal stick-out
- Tool runout checked (end mills)
- Suitable coolant (or air for some operations)
- Chip evacuation (no re-cutting)
- Planned tool change before breakage
FAQ
Should you always use coolant?
No: some carbide milling operations do better with air or dry (less thermal shock). Follow the tool maker’s recommendation.
Why does a new end mill break right away?
Often runout, stick-out, too abrupt an entry or too thick a chip; see Milling troubleshooting.
Sources
- Sandvik Coromant — Wear on cutting edges, consulted November 26, 2026.
- Sandvik Coromant — How to improve tool life in turning, consulted November 26, 2026.
- Johansson et al. — Assessment of different tool life models (Lund University, PDF), consulted November 26, 2026.
One guide a week, French-first