CoupeFab

Fundamentals · plasma

Lead-ins, lead-outs, pierce height and pierce delay in plasma cutting

Where to place the lead-in, what shape to give it, why pierce higher than cut height, how to set the delay, and clean holes — with the values that come from your chart.

Reviewed 3 min read Level : Intermediate DraftWritten by CoupeFab from the official documents cited. Technical review by Michaël Brassard pending.

Piercing is the hardest moment for consumables: molten metal is blown back toward the torch before the arc breaks through. The lead-in then carries the stabilized arc to the contour, and the lead-out ends it without marking the part. Set well, they make the difference between a clean part and a part to grind.

The settings and where they come from

SettingJobSource of the value
Pierce heightProtect the torch from spatterYour source’s cut chart (often expressed relative to cut height)
Pierce delayLet the arc break through before movingCut chart, by thickness
Cut heightDistance while cuttingCut chart
Arc voltage (THC)Height controlChart; automatic mode depends on the control
Lead-in lengthStable arc before the contourTesting; depends on thickness and pierce

Where to place the lead-in

  1. Scrap side. For an outside profile, the lead-in starts in the scrap; for a hole, it starts inside the hole (which will drop).
  2. Away from functional edges. Avoid a datum face, a precision hole or a visible edge; the entry point almost always leaves a mark.
  3. Into a corner when possible. On an outside profile, entering near a corner hides the mark.
  4. Far enough from the contour. The pierce crater must sit entirely in the scrap.
  5. Cut order. Small inside features first, outside profile last, so the part does not move before the end.

Lead-in and lead-out shapes

ShapeTypical use
Straight perpendicularSimple, outside profiles
Tangent arcHoles and profiles where you want to avoid a nick
Line + arcCommon compromise in plasma CAM
Short or no lead-out, small overcutAvoid a gouge at the closing point

Too long an overcut gouges the part; too short leaves a tab. Tune it by testing in small steps.

Cut direction

The plasma jet swirls: one side of the kerf is squarer than the other. With a standard swirl ring (clockwise), the right side in the direction of travel is usually the good side: cut outside profiles clockwise and holes counter-clockwise. Check your manual: some consumables swirl the other way.

Clean holes

  • Small plasma holes show more bevel and taper. Manufacturers publish guidance (minimum diameter relative to thickness, reduced speed, THC off in the hole); Hypertherm, for example, markets True Hole technology on some high-end systems.
  • Disable or lock the THC on small holes and in corners (the control’s anti-dive function): speed drops, voltage rises, the torch would dive.
  • For a precise functional hole: drill or ream afterward, or go to laser.

Piercing thick plate

Beyond the maker’s stated pierce capacity, use a moving pierce or an edge start. Pierce capacity is lower than the advertised cut capacity: read both numbers on the source’s spec sheet.

Common mistakes

SymptomLikely cause
Nozzle and shield wear fast, stuck spatterPierce height too low or delay too short
No break-through, arc goes outDelay too short for the thickness
Crater bites into the partLead-in too short or badly placed
Nick at the closing pointOvercut too long, lead-out badly oriented
Torch dives in holesTHC active at low speed

FAQ

Do I need a lead-in for marking?

No: marking runs at low current without a through pierce. Use the CAM marking operation.

Longer delay = safer?

Not necessarily: too long a delay widens the crater and wears the nozzle. Follow the chart, then tune by testing.

Sources

Spotted an error or want something added? Tell us →

One guide a week, French-first

New guides, used equipment in Quebec and price moves. No third-party ads.

CASL compliance: the box is not pre-checked. Nothing is sent without this express consent.