CNC router: eliminating tear-out and chipping in plywood and melamine
Choosing between upcut, downcut and compression bits, setting a compression bit’s first pass, ramping in, and diagnosing chipping on the top or bottom face of the sheet.
Router tear-out (chipped veneer, lifted fibers) comes mostly from the bit’s helix direction relative to the visible face, then from wear and cutting conditions. The good news: most of it is fixed by picking the right geometry and using it correctly.
Upcut, downcut or compression
| Geometry | Effect | Good for | Watch out |
|---|---|---|---|
| Upcut | Lifts chips, good evacuation | Soft and hard woods, plastics, foam; deep slots | Can tear the top face and lift the part if vacuum is weak |
| Downcut | Pushes down, clean top, part held down | Softwood, composites (MDF, veneered plywood, particleboard); shallow pockets | Chips repacked in the cut, heat |
| Compression | Upcut at the tip, downcut above: both faces squeezed toward the middle | Sheets veneered or laminated on both sides, through cuts | Pointless if the pass is shallower than the upcut section |
The compression-bit rule
The first pass must be deeper than the bit’s upcut section (often about 6 mm, or ¼ in, depending on the model: check the maker’s data). Otherwise only the upcut part works on the top face, which tears as with an upcut bit. Ideally cut in one full-depth pass when the machine and hold-down allow.
Quick diagnosis
| Symptom | Likely cause | Fix |
|---|---|---|
| Chipping on the top | Upcut bit, or compression too shallow | Downcut or compression, first pass deeper than the upcut section |
| Chipping on the bottom | Downcut bit breaking through | Compression or upcut; spoilboard in good shape |
| Fuzzy edges everywhere | Worn edge, chip load too low (rubbing) | New tool; raise feed or lower RPM (see Feeds and speeds) |
| Burnt edges | Repacked chips, feed too slow | Ramp, better dust collection, higher feed |
| Parts moving | Upcut + weak vacuum | Downcut/compression, tabs, tape or screws |
Common mistakes
- Shallow pocketing with a compression bit: use a downcut.
- Lowering feed “for a better finish”: the bit rubs, heats and wears faster.
- Keeping a worn bit on melamine, which is unforgiving.
Checklist
- Geometry suits the material and the visible face
- Upcut section length known (maker’s data)
- First pass deeper than that length
- Ramped entries; dust collection on
- Spoilboard flat and in good shape
FAQ
Compression for MDF?
Possible, but MDF is very abrasive: many shops keep an upcut for raw MDF and save compression bits for veneered or melamine sheets.
Why does my compression bit still tear out?
Almost always because the pass is shallower than the upcut section, or the tool is worn.
Sources
- C.R. Onsrud — Finding the Right Tool for the Job on Your CNC Router: upcut, downcut and compression effects. Consulted November 26, 2026.
- AXYZ — How to Use a Compression Bit: compression principle, ramping in.
- Popular Woodworking — Compression Bits (CNC Tooling Basics, part 3): first pass deeper than the upcut section.
One guide a week, French-first
New guides, used equipment in Quebec and price moves. No third-party ads.